Excessive Restraint Causes Cold Cracking in Heavy Plate Welding

E42-011 · Weld Distortion & Defects · Pressure Vessel Cylindrical Shell Butt Joint · ★★★

Problem Symptom

Delayed cracking found 24h after welding, the whole batch has to be reworked

Root Cause

[Restraint Stress] For thick plate t=40mm with strong restraint, the restraint rigidity R=5000N/mm and the blocked shrinkage stress is σ_r=R×αΔT≈400MPa.
[Cold Cracking Criterion] Carbon equivalent CE=0.45 and diffusible hydrogen [H]=8ml/100g, so the cold cracking sensitivity index exceeds the threshold.
[Design Omission] No preheat was applied (120℃ required) and no post-weld heat treatment was used.

Correct Solution

1) Preheat to 120℃ before welding and control the interpass temperature;
2) Use low-hydrogen consumable J507RH baked at 350℃;
3) Bake after welding for dehydrogenation at 250℃×2h;
4) Reduce restraint (add shrinkage allowance);
5) Inspect by NDT 48h after welding;
6) Control the assembly gap to ≤2mm;
7) Keep the ambient humidity ≤80%;
8) Make the PQR welding procedure qualification a mandatory pre-welding confirmation.

Checklist

References

NB/T 47014 Welding Procedure Qualification for Pressure Equipment

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »