Undersized Bevel Causes Lack of Penetration in Heavy Plate

E42-012 · Weld Distortion & Defects · Box Column Main Weld Seam · ★★★

Problem Symptom

UT inspection shows incomplete penetration 4mm deep, load capacity insufficient

Root Cause

[Bevel Section] The V-bevel angle β=35° (60° required) and the root face p=8mm is too large, so the effective penetration depth is insufficient.
[Penetration Check] For single-side welding the penetration depth is d=0.7×t_w×√I≈16mm, less than the 20mm plate thickness, leaving 4mm of unfused root.
[Design Omission] The bevel design was wrong and double-side welding was not used.

Correct Solution

1) Change the bevel to an X-shape with 60° angle and root face ≤3mm;
2) Use double-side welding to guarantee penetration;
3) Add a gouging operation;
4) Determine the welding parameters through penetration trials;
5) Inspect every seam by UT until qualified;
6) Verify penetration depth on the first article by sectioning;
7) Require welders to hold valid certificates;
8) Include bevel preparation and penetration verification in the welding first-article inspection.

Checklist

References

GB/T 11345-2013 Ultrasonic Testing of Welds