E42-060 · Weld Distortion & Defects · Construction Machine Boom Q345 · ★★
Heat-affected zone embrittlement, Charpy impact energy KV2<27J
[Welding Heat Input] With a current of 280A, a voltage of 28V and a speed of 25cm/min, the heat input E=60UI/v=60×280×28/250=1884J/mm, far too high.
[Overheated Structure] E>1500J/mm grows the HAZ grains to ASTM grain size 2 and the Charpy impact energy KV2<27J fails the requirement.
[Design Omission] The heat input was not limited to ≤25kJ/cm and the interpass temperature was not controlled, giving a high risk of brittle cracking.
1) Limit the heat input to ≤25kJ/cm;
2) Use multi-layer multi-pass welding to reduce the heat input;
3) Control the interpass temperature at 80-150℃;
4) Normalise after welding to refine the grains;
5) Require Charpy impact energy KV2≥27J at -20℃;
6) Carry out a welding procedure qualification;
7) Test the HAZ hardness;
8) Write the heat input into the WPS.
GB/T 19866-2003 Welding Procedure Specification