Knowledge Base › Structural Design Error Case Study › Quenched-and-Tempered Steel Excessive Welding Current Causing HAZ Softening Sag

Quenched-and-Tempered Steel Excessive Welding Current Causing HAZ Softening Sag

E42-266 · Welding Deformation and Defects · Quenched-and-Tempered Steel Component · ★★

Problem Description

Quenched-and-tempered steel component (40Cr QT HB280) weld HAZ hardness drops from 320HB to 240HB; local sag 2mm after loading; 5 pieces reworked per month

Root Cause

[Overheat Softening] Excessive welding current; heat input reaches 28kJ/cm (should be ≤15kJ/cm); HAZ temper-softened band width b=4mm; hardness drops from 320HB to 240HB.
[Strength Drop] Softened zone yield σs=780MPa below working stress σ=850MPa; local sag δ=2mm after loading.
[Design Omission] Heat input not controlled; no post-weld tempering; safety factor 1.1 (should be ≥1.6); no HAZ hardness test.

Corrective Solution

1) Limit heat input to ≤15kJ/cm; multi-pass small current;
2) Preheat base metal 150℃ to lower cooling rate;
3) Post-weld dehydrogenation 200℃×2h;
4) Hardness test HAZ pass by pass (≥300HB);
5) Local post-weld tempering 520℃ to restore QT condition;
6) Optimize groove to reduce deposition by 30%;
7) Sample softened band each batch;
8) Re-inspect sagged parts after straightening.

Checklist

Reference

GB/T 19869.1-2005

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL