Knowledge Base › Structural Design Error Case Study › Stainless Steel Excessive Interpass Temperature Causing Coarse Grain and Toughness Drop

Stainless Steel Excessive Interpass Temperature Causing Coarse Grain and Toughness Drop

E42-268 · Welding Deformation and Defects · 304 Stainless Tank · ★★

Problem Description

304 stainless tank weld zone coarse grains; impact energy KV2 only 28J (should be ≥60J); 4 units reworked per month

Root Cause

[Overheat Coarse Grain] Interpass temperature controlled to 200℃ (should be ≤150℃); heat input q=22kJ/cm too high; grains grow to ASTM grade 3 (should be ≥grade 5).
[Toughness Drop] Grain boundary carbide aggregation; impact energy KV2=28J only 47% of spec.
[Design Omission] Interpass temperature not controlled; no grain size test; safety factor 1.3 (should be ≥1.8).

Corrective Solution

1) Limit interpass temperature to ≤150℃; measure pass by pass;
2) Small current fast welding q≤15kJ/cm;
3) Argon backing protection to prevent oxidation;
4) Post-weld solution treatment at 1050℃;
5) Sample grain size each batch ≥grade 5;
6) Impact test each batch (≥60J);
7) Optimize sequence symmetric welding;
8) Cooling water temperature control to prevent overheating.

Checklist

Reference

GB/T 20878-2007

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL