Air Entrainment by the Gating System Causes Gas Porosity in the Casting

E42-014 · Casting Defects · Aluminium Cylinder Head (ZL104) · ★★★

Problem Symptom

Dense gas pores Φ2mm on the machined face, gas tightness not qualified

Root Cause

[Entrainment Mechanism] The sprue is not filled fully and backflow draws in air, so the entrained gas volume Q∝v²×A=0.4L per part.
[Porosity Formation] Venting of the mould cavity is poor, so the gas is trapped by the metal and solidifies into pores, with a porosity rate of 1.2%.
[Design Omission] The gating system has no filter and no vent, so gas tightness fails.

Correct Solution

1) Adopt a bottom-filling gating system to prevent entrainment;
2) Fit a filter and a slag trap;
3) Add vents and vent pins;
4) Keep the mould sand permeability ≥80;
5) Replace gravity casting with low-pressure casting;
6) Radiographically inspect the machined face before machining;
7) Optimise the pouring speed;
8) Include the gating system parameters in the casting first-article verification.

Checklist

References

GB/T 1173 Casting Aluminium Alloys

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL