E42-272 · Casting Defects · Machine Tool Bed · ★★
The machine tool bed casting surface locally swells with oversize metal 3mm thick, dimensions out of tolerance; 8 parts reworked per month
[Uneven Compaction] Local sand compaction is only 60% (should be ≥85%); iron static head p=ρgh crushes the mold wall, causing swell.
[Oversize Metal] Surface swell 3mm thick; the 1.5mm machining allowance is insufficient, causing out-of-tolerance dimensions.
[Design Omission] Compaction not controlled, no cast-iron liners in the cavity; dimensional tolerance only IT15 (should be IT12).
1) Keep sand compaction uniformly ≥85% and inspect;
2) Add cast-iron liners in the cavity for location;
3) Optimize the parting surface to reduce loose pieces;
4) Raise green compressive strength of sand to 0.12MPa;
5) Measure compaction per mold;
6) Leave machining allowance on the pattern ≥3mm;
7) Limit pouring rate to reduce dynamic pressure;
8) Sampling-check key dimensions each batch.
GB/T 9442-2010