E42-395 · Casting Defects · HT250 Bed · ★★
The HT250 bed thin wall (8mm) is not filled, with missing metal; 2 parts scrapped per month
[Misrun] Pouring temperature 1280℃ is too low, poor fluidity.
[Missing Metal] Far-end wall missing.
[Design Omission] Pouring temperature not raised, wall too thin; safety factor 1.4.
1) Raise pouring temperature to 1380℃;
2) Thicken thin walls to 12mm;
3) Add overflow risers;
4) Speed up pouring;
5) Section the first piece each batch;
6) Increase pattern draft;
7) Control sand moisture;
8) Composition control.
GB/T 9439-2010