Insufficient Tempering Causes Grinding Cracks

E42-017 · Heat Treatment Distortion & Cracking · Bearing Ring (GCr15) · ★★★

Problem Symptom

Network cracks appear on the surface after grinding, the whole batch is scrapped

Root Cause

[Retained Austenite] After quenching and tempering at 150℃×1h the retained austenite AR=15% (it should be ≤5%) and has not fully transformed.
[Grinding-Induced Cracking] The 200℃ grinding heat transforms AR to martensite with volume expansion, and the grinding tensile stress σ_t=600MPa exceeds σ_f=450, producing a network of cracks.
[Design Omission] The tempering process was wrong and AR was not controlled, so the part cracked.

Correct Solution

1) Raise tempering to 180℃×3h for full transformation;
2) Add a second ageing step to stabilise the structure;
3) Control AR≤5% by XRD;
4) Use a CBN wheel with a small infeed v=15m/s for grinding;
5) Provide adequate cooling to prevent heat build-up;
6) Inspect 100% by magnetic-particle testing;
7) Control hardness uniformity;
8) Include the AR test in the final heat treatment inspection.

Checklist

References

GB/T 18254 High Carbon Chromium Bearing Steel