Non-Uniform Carburised Case Depth Causes Tooth Surface Spalling

E42-018 · Heat Treatment Distortion & Cracking · Heavy-Duty Gear (20Cr2Ni4) · ★★★

Problem Symptom

Tooth surface spalling after 6 months of running, with a risk of tooth breakage

Root Cause

[Case Depth Deviation] The carburised case depth is uneven at 0.6-1.4mm (1.2±0.1 required) and only reaches 0.6mm in the thin areas.
[Contact Fatigue] In the thin-layer zone the contact stress σ_H=1500MPa consumes the margin against the allowable 1600 for that depth, and the spalling pits extend into the substrate.
[Design Omission] The carburising furnace temperature field was non-uniform and the case depth was not checked, so the tooth surface spalled.

Correct Solution

1) Keep furnace temperature uniformity within ±5℃;
2) Control the case depth to 1.2±0.1mm;
3) Add a post-carburising diffusion homogenising step;
4) Optimise the tooth surface hardness gradient;
5) Use closed-loop control of the carbon potential;
6) Sample the case depth for metallographic examination;
7) Inspect the tooth surface by NDT;
8) Include the case depth distribution in the first-article carburising qualification.

Checklist

References

GB/T 8539 Gear Materials and Heat Treatment

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL