Non-Uniform Water Quenching of a Cylinder Tube Causes Ovality of the Bore

E42-066 · Heat Treatment Distortion & Cracking · Cylinder Tube 45 Steel · ★★

Problem Symptom

Bore ovality 0.05mm (allowable 0.01)

Root Cause

[Non-Uniform Cooling] With a wall thickness difference, the thin wall cools and shrinks first during water quenching, making the bore oval by Δ=0.05mm.
[Oval Deformation] A cooling rate difference of 3 times causes non-uniform shrinkage, so the bore exceeds tolerance by 5 times.
[Design Omission] Stepped quenching was not used and the bore was not round-ground, so the part was reworked.

Correct Solution

1) Change to stepped quenching or oil quenching;
2) Fit a mandrel in the bore before quenching to constrain it;
3) Quench with uniform spraying;
4) Round-grind the bore after quenching;
5) Leave 0.3mm of grinding allowance in the bore;
6) Test the hardness gradient;
7) Temper sufficiently to relieve stress;
8) Include the deformation check-up in the process.

Checklist

References

GB/T 16924-2008 Steel Parts — Quenching and Tempering