Improper Slow Cooling After Carburising Causes Network Cementite in the Gear Shaft

E42-067 · Heat Treatment Distortion & Cracking · Gear Shaft 20CrMnTi · ★★

Problem Symptom

Network carbides in the case, the teeth crumble during grinding

Root Cause

[Improper Slow Cooling] After carburising the part is furnace-cooled to 600℃ and air cooled, so network Fe₃C precipitates along the grain boundaries.
[Embrittlement] The network carbides reduce the impact toughness and the teeth crumble during grinding.
[Design Omission] No normalising was done to eliminate the network and the part was quenched directly, so the teeth broke.

Correct Solution

1) Normalise after carburising to eliminate the network;
2) Control the cooling rate;
3) Rate the carbide level at ≤grade 3;
4) Perform a structure pretreatment before quenching;
5) Split the grinding allowance into rough and finish passes;
6) Keep the case depth at 1.2-1.6mm;
7) Perform metallographic inspection;
8) Include the normalising in the process.

Checklist

References

GB/T 16923-2008 Steel Parts — Normalising

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »
MOULDL · Mechanical Engineering Knowledge Base · free self-study reference for machine designers, 3D CAD models at MOULDL