E42-277 · Heat Treatment Distortion and Cracking · Thin Spring Sheet · ★★
Thin spring sheets (1.5×60×400) over-densely loaded heat unevenly and warp 2mm after discharge; 12 parts reworked per month
[Dense Loading] Part spacing only 5mm (should be ≥30mm); local over-temperature 20℃; temperature difference ΔT causes warpage.
[Thermal Distortion] Temperature difference causes warpage δ=α·L·ΔT≈2mm, exceeding flatness 0.5mm.
[Design Omission] Loading not controlled, no dedicated fixture; flatness only IT14 (should be IT9).
1) Keep part spacing ≥30mm;
2) Hang with dedicated racks for uniform temperature;
3) Load in the uniform-temperature zone;
4) Temperature control accuracy ±5℃;
5) Measure distortion ≤0.5mm per furnace;
6) Press-quench to prevent warpage;
7) Aging to set shape;
8) CMM recheck of the first piece.
GB/T 16923-2008