Knowledge Base › Structural Design Error Case Study › Nitriding Furnace Temperature Fluctuation Causing Case-Depth Variation and Dimensional Scatter

Nitriding Furnace Temperature Fluctuation Causing Case-Depth Variation and Dimensional Scatter

E42-278 · Heat Treatment Distortion and Cracking · Precision Lead Screw · ★★

Problem Description

The precision lead screw (Tr40×6) shows nitrided case-depth variation 0.1mm, causing assembly interference within a batch; 6 parts reworked per month

Root Cause

[Temperature Fluctuation] Nitriding furnace temperature fluctuates ±15℃ (should be ±5℃); case depth difference Δh=0.1mm.
[Dimensional Scatter] Expansion varies among parts in the batch; fit clearance scatters 0.08mm, causing interference.
[Design Omission] Furnace temperature not calibrated, ammonia dissociation not controlled (should be 35%~45%); dimensional consistency CPK<1.0.

Corrective Solution

1) Calibrate furnace temperature to ±5℃;
2) Control ammonia dissociation to 35%~45%;
3) Clean and degrease before loading;
4) Measure case depth on furnace coupons each batch;
5) Sampling case depth ±0.02mm;
6) Upgrade temperature control system with recording;
7) Freeze process parameters;
8) Recheck first-piece dimensions.

Checklist

Reference

GB/T 18177-2008