Knowledge Base › Structural Design Error Case Study › Slow Stack Cooling After Normalizing Causing Coarse Pearlite and Low Strength

Slow Stack Cooling After Normalizing Causing Coarse Pearlite and Low Strength

E42-279 · Heat Treatment Distortion and Cracking · Steel Casting · ★★

Problem Description

The ZG270-500 steel casting after normalizing has coarse pearlite lamellae, σb=520MPa (should be ≥600), low strength; 8 parts reworked per month

Root Cause

[Slow Cooling] Normalized stack cooling; cooling rate only 0.5℃/s (should be ≥1.5); pearlite coarsens with interlamellar spacing >0.3μm.
[Strength Loss] σb=520MPa (should be ≥600); yield ratio drops.
[Design Omission] No forced air cooling, cooling rate not controlled; strength margin only 0.87 (should be ≥1.1).

Corrective Solution

1) Forced air cooling after normalizing;
2) Control cooling rate ≥1.5℃/s;
3) Variable-speed fans;
4) Metallography each batch (pearlite lamellae ≤0.2μm);
5) Recheck strength ≥600MPa;
6) Reduce loading density;
7) Freeze the process card;
8) First-piece mechanical test.

Checklist

Reference

GB/T 16923-2008

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »