E42-420 · Stress Concentration · Φ1200 Ammonia Sphere Nozzle · ★★★
Φ1200 ammonia sphere DN200 nozzle fillet weld r=1mm stress-corrosion crack; ammonia leak; handled at annual survey
[Small Fillet] Nozzle fillet r=1mm (should be ≥6mm); Kt=2.6. [SCC] Tensile stress + ammonia medium; intergranular crack. [Design Omission] Not ground smooth; no PWHT; safety factor 1.2 (should be ≥2.0).
1) Grind nozzle fillet R≥6mm;
2) Overall PWHT after welding;
3) Fillet weld MT+UT;
4) Switch to corrosion-resistant steel;
5) Limit operating stress;
6) Add online monitor;
7) Coat inner wall;
8) Periodic NDE.
GB/T 150.1-2011