Weld Sensitisation of a Stainless Steel Tank Causes Intergranular Corrosion Cracking

E42-078 · Corrosion Failures · Stainless Steel Tank 06Cr19Ni10 · ★★★

Problem Symptom

Intergranular corrosion cracks in the weld heat-affected zone

Root Cause

[Sensitisation] The welding thermal cycle of 450-850℃ causes Cr23C6 to precipitate at the grain boundaries and the chromium-depleted zones form.
[Intergranular Corrosion] The chromium-depleted grain boundaries corrode selectively in the medium and crack.
[Design Omission] Ultra-low-carbon or stabilised steel was not used and no solution treatment was applied, so the tank cracked and leaked.

Correct Solution

1) Change to ultra-low-carbon 304L or 321 stabilised steel;
2) Apply solution treatment after welding;
3) Weld with low heat input at high speed;
4) Carry out an intergranular corrosion test (copper sulphate);
5) Control chloride in the medium to ≤25ppm;
6) Match the consumables;
7) Apply passivation treatment;
8) Include corrosion-resistant material selection in the design.

Checklist

References

GB/T 4334-2020 Stainless Steels — Intergranular Corrosion Test

Related 3D models: Ready to build it? Download free 3D models & CAD drawings at MOULDL »