E42-128 · Corrosion Failures · Desulphurisation Pump Outlet Elbow · ★★★
The outer arc of the elbow thins to 2mm (originally 8mm), perforates and leaks
[Erosion Corrosion] A high-velocity slurry containing solids scours the outer arc of the elbow in synergy with corrosion, giving a high thinning rate.
[Perforation] The outer arc wall thins to the critical value and perforates.
[Design Omission] The elbow had no wear-resistant lining and the flow velocity was too high.
1) Line the elbow internally with wear-resistant ceramic or rubber;
2) Reduce the medium velocity to ≤3m/s;
3) Thicken the outer arc to 12mm;
4) Install online wall thickness monitoring;
5) Perform periodic thickness sampling;
6) Optimise the flow path by simulation;
7) Rotate spare elbows in service;
8) Include erosion corrosion in the patrol inspection.
GB/T 50050 Code for Design of Industrial Recirculating Cooling Water Treatment