E42-434 · Corrosion Failure · 2000m³ diesel tank bottom plate · ★★★
2000m³ diesel tank bottom plate (edge plate): soil corrosion perforation and oil seepage; treated annually
[Soil corrosion] Oxygen concentration cell between edge plate and foundation, corrosion rate 0.2mm/a. [Perforation] Bottom plate 8mm thick, perforated in 10 years. [Design Omission] No cathodic protection, no waterproof layer; safety factor 1.2 (should be ≥2.0).
1) Add cathodic protection to bottom plate;
2) Add waterproof asphalt layer on edge plate;
3) Change material to Q345R plus coating;
4) Flux-leakage test every 2 years;
5)FoundationDrainage;
6) Thicken edge plate;
7) On-line monitoring;
8) Periodic tank cleaning.
GB 50341-2014