E42-438 · Corrosion Failure · DN200 oil pipeline · ★★★
DN200 buried oil pipeline: stray-current corrosion, local perforation and leak; repaired twice a year
[Stray-current corrosion] Current discharged from nearby cathodic station, local corrosion rate 0.5mm/a. [Perforation] Wall 6mm thick, perforated in 3 years. [Design Omission] No insulation, no drainage; safety factor 1.2 (should be ≥2.0).
1) Add insulating joints to pipeline;
2) Provide drainage grounding;
3) Reinforce external corrosion-protection coating;
4) Close-interval survey every 2 years;
5)Potential monitoring;
6)Cathodic protection;
7) Route away from interference sources;
8) Periodic excavation sampling.
GB/T 21447-2018