E42-477 · Corrosion Failure · Buried steel pipe · ★★
Buried steel pipe (φ219): external corrosion perforation and leak, shut down; repaired once a month
[External corrosion] Coating damaged, soil resistivity ρ=20Ω·m causing corrosion perforation.
[Hole] Wall thinned by corrosion.
[Design Omission] No cathodic protection, no leak detection; safety factor 1.3 (should be ≥2.5).
1) External epoxy coal-tar pitch coating;
2) Add impressed-current cathodic protection;
3) Pipeline NDE and thickness measurement;
4) Control soil corrosion;
5) Leak detection annually;
6) Raise wall thickness to 8mm;
7) Add protective sleeve;
8) Periodic re-measurement.
GB/T 21447-2018