E42-528 · Corrosion Failure · Seawater cooler · ★★★
Tube bundle φ19×2: chloride pitting perforation and leak; replaced once a year
[Pitting] Cl-=20000ppm, passive film broken, pitting rate 0.5mm/a.
[Material] 304 not chloride-resistant.
[Design Omission] No duplex steel, no corrosion inhibitor; safety factor 1.2 (should be ≥2.0).
1) Change to 2205 duplex steel;
2) Add corrosion inhibitor;
3)Cathodic protection;
4) Leak check monthly;
5) Limit Cl-;
6) Coat/plate;
7) Control flow velocity;
8) Periodic thickness measurement.
GB/T 24511-2017