Liquid Nitrogen Cooling Too Deep Causes Brittle Fracture of the Shaft

E43-165 · Interference Fit Failures · Gear Shaft ∅60, liquid nitrogen cooling specified at -196℃ but measured -150℃, excessive · ★★

Problem Symptom

The excessive cold caused the toughness of the 40Cr shaft to drop and the shoulder root cracked under the assembly impact

Root Cause

[Mechanism] Excessive deep cooling shifted the ductile-to-brittle transition temperature upward, so the impact toughness fell sharply and the part fractured.
[Calculation] The required contraction Δ=αLΔT=12e-6×60×ΔT≥0.15 needs ΔT≥208℃, that is ≤-188℃; the measured -150℃ gave Δ=0.11mm, which is insufficient, and the cooling was excessive.
[Design Omission] The upper limit of the cooling temperature and the warm-up time were not specified; this design flaw caused brittle fracture.

Correct Solution

1) Control the cooling to -78~-120℃;
2) Limit the depth of cooling;
3) Add a warm-up stage;
4) Select a tough steel;
5) Fit it slowly;
6) Carry out NDT after cold assembly to check the mating surface for cracks;
7) Control the impact;
8) Carry out a cold test on the first piece.

Checklist

References

GB/T 5371-2004 Interference Fits — Calculation and Selection