E43-172 · Interference Fit Failures · Dryer Section Shaft ∅150, interference 0.10mm, working temperature 180℃, steel-to-cast-iron dissimilar materials · ★★
At high temperature the cast iron expanded more than the steel so the interference disappeared and the dryer came loose
[Mechanism] The difference in linear expansion coefficients between dissimilar materials reduced the contact pressure at high temperature and could even turn the fit into a clearance.
[Calculation] Δinterference=αiron LΔT-αsteel LΔT=(12-11)e-6×150×180=0.027mm, so the original 0.10 became 0.073 and was still tight; if the cast iron had been looser the fit would have failed.
[Design Omission] No hot-state interference compensation was made and the materials were mismatched; this design flaw caused loosening.
1) Add +0.05mm hot-state interference;
2) Use the same material on both parts;
3) Limit the assembly heating temperature to prevent material annealing;
4) Control the press force;
5) Monitor the assembly temperature with a thermometer;
6) Carry out NDT after hot assembly to check for cracks;
7) Re-tighten the locking parts after hot operation;
8) Carry out a hot test on the first piece.
GB/T 5371-2004 Interference Fits — Calculation and Selection