E43-096 · Weld/Cast Forming Out of Tolerance · Machine Column Welding · ★★★
Weld distortion shifted the hole positions by 0.30, leaving insufficient boring allowance
[Weld Distortion] The welding heat bowed the column so the hole positions shifted 0.30.
[Insufficient Allowance] The distortion reduced the boring allowance below 0.5mm, so the holes were off position.
[Design Omission] The part should have been pre-distorted before welding and aged after welding, but no distortion pre-control was applied.
1) Apply pre-distortion before welding;
2) Weld in segments symmetrically;
3) Stress relieve after welding;
4) Leave 1.0 of machining allowance;
5) Qualify the welding process;
6) Inspect the first piece on a CMM;
7) Correct weld distortion mechanically after welding;
8) Weld repair and re-bore out-of-specification parts.
GB/T 19804-2003 General Tolerances for Welded Structures