E43-351 · Welded/Cast Forming Dimensional Error · An HT250 reducer housing 1200mm long, designed two-bearing hole spacing 1200±0.05, measured post-cast distortion 1200.32 · ★★
Release of casting residual stress deforms the housing, pushing the hole spacing 0.32mm out of tolerance and causing gear-mesh noise.
[Mechanism] Uneven wall thickness and uneven cooling create casting residual stress; after roughing removes the constraint, the stress releases and shifts the hole pattern.
[Calculation] Hole-spacing deformation Δ≈σ_res·L/E=40×1200/110000≈0.44mm; the measured 0.32mm is 6× the 0.05mm tolerance.
[Design Omission] No symmetric wall thickness or adequate aging — a design defect leading to hole-spacing error.
1) Before roughing, naturally age ≥6 months or vibratory-stress-relieve to remove stress;
2) Use symmetric wall thickness to reduce the cooling-stress difference;
3) Insert a second aging step between rough and finish machining;
4) Before machining, use a bridge plate to set the hole-spacing datum;
5) Provide evenly distributed process pads to balance material removal and reduce distortion;
6) Temper after roughing to remove residual stress;
7) Re-check hole spacing on a CMM;
8) Verify first-article hole spacing ≤0.05mm.
GB/T 9439-2010 Grey cast iron castings