E44-967 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Wrong material, corrosion, leakage
[Mechanism] A vessel handling chloride service was mistakenly built in carbon steel; pitting and stress corrosion thinned the wall until it leaked.
[Calculation] Fluid Cl- 5000ppm, carbon-steel corrosion rate 1.2mm/a, wall loss 2.4mm over 2 years, and perforation leak.
[Design Omission] No corrosion-resistant material chosen, no fluid compatibility check, and no lining.
1) Re-select 316L stainless steel (resists Cl- to 20000ppm), since carbon steel corrodes fast and a better steel resists it — thus preventing corrosion;
2) Check material-fluid compatibility (per the GB/T 150 corrosion table), since an incompatible metal corrodes and a check assures it — thus compliant selection;
3) Line with PTFE (3mm thick), since a bare wall corrodes and a liner isolates it — thus isolating corrosion;
4) Run coupon testing (verify corrosion rate ≤0.05mm/a), since a wrong choice causes corrosion and measurement confirms resistance — thus setting selection by data;
5) Perform periodic thickness measurement (every six months), since thinning first shows as wall loss and can be replaced early — thus monitoring thickness;
6) Run a hydrotest (verify no leak), since leaks were never tested and measurement confirms sealing — thus confirming sealing;
7) In operation, hold Cl-≤50ppm (treat if exceeded), since corrosion rises with concentration and fluid control suppresses it — thus running to prevent corrosion;
8) Write material selection and compatibility into the spec, since the corrosion root cause was the wrong selection unchecked — thus locking it in by specification.