E44-968 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Creep bulging, diametral growth, deformation
[Mechanism] The vessel ran long-term above the material's creep temperature; creep deformation grew and thinned the shell, lowering strength.
[Calculation] Operating at 480℃ (carbon-steel creep temperature 420℃), after 5 years the shell grew 3% in diameter and the wall thinned 1.5mm.
[Design Omission] No creep-life check, no heat-resistant material, and no temperature control.
1) Check creep life (Larson-Miller gives t_r≥10 years, was under 5), since exceeding creep causes bulging and the life check shows margin — thus preventing bulging;
2) Choose 15CrMoR heat-resistant steel (creep limit 540℃), since carbon steel softens and bulges while a better steel resists creep — thus selecting the material;
3) Lower the operating temperature below 420℃ (was 480℃), since high temperature bulges and cooling suppresses it — thus suppressing creep;
4) Thicken the wall to δ=14mm (was 10mm), since a thin wall bulges fast and a thicker one slows it — thus reinforcing;
5) Run creep testing (verify growth rate ≤0.2%/a), since creep was never checked and measurement confirms the rate — thus setting creep life by data;
6) Perform periodic thickness measurement (annual, replace on growth), since creep first shows as bulging and can be replaced early — thus monitoring bulge;
7) In operation, hold temperature ≤420℃ (reduce if exceeded), since high temperature bulges and temperature control prevents growth — thus running to prevent bulge;
8) Write the creep check and material selection into the calculation book, since the bulge root cause was operation above creep temperature unchecked — thus locking it in at design.
GB/T 150.1-2011 Pressure vessels