E44-969 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★
Low temperature, brittle fracture, cracking
[Mechanism] Below the ductile-to-brittle transition temperature, the Charpy impact energy of carbon steel collapses, and cracks propagate without plasticity in a brittle fracture.
[Calculation] Design temperature Td=-29℃ is below Q235B's allowable -20℃; at -29℃ the impact energy is only 18J (needs ≥27J). Fracture toughness KIC=32MPa·m^0.5, critical crack size aC=KIC²/(1.21πσ²)=32²/(1.21π×120²)=19mm, smaller than the measured 25mm defect.
[Design Omission] No low-temperature impact test, no critical-crack-size check, and no post-weld heat treatment.
1) Switch to Q345R with a -40℃ impact report (energy ≥31J), since the original Q235B at -29℃ gave only 18J, below the 27J threshold, and a better steel restores toughness — thus preventing brittle fracture;
2) Accept with Charpy V impact per GB/T 150.1 (samples at design temperature +0℃, ≥31J), since room-temperature acceptance could not confirm low-temperature toughness and impact testing quantifies it — thus locking it in at acceptance;
3) Hold the minimum operating temperature ≥-20℃ (limit production below that), since below the transition temperature cleavage fracture occurs and limiting temperature avoids the risk — thus running to prevent fracture;
4) Post-weld overall stress-relief annealing (620℃×2h), since weld residual stress raised the effective stress to 180MPa and annealing drops it to 90MPa — thus raising aC to prevent cracking;
5) 100% radiograph the weld and HAZ (Class II acceptance), since the uninspected 25mm defect >aC 19mm and early rejection removes the source — thus weeding out over-limit defects;
6) Re-verify with -29℃ low-temperature impact (3 pieces per heat), since there were no low-temperature data and re-testing confirms design-temperature toughness — thus grading by data;
7) Hold the pressurization rate ≤0.3MPa/min (slow any fast ramp), since dynamic load triggers brittle cracking and a slow ramp is steady — thus operating smoothly;
8) Write low-temperature material selection and impact acceptance into the technical spec, since the brittle-fracture root cause was missing low-temperature steel and impact testing — thus locking it in by specification.
GB/T 150.1-2011 Pressure vessels