Knowledge Base › Fluid Systems Error Case › Stress-Corrosion Cracking

Stress-Corrosion Cracking

E44-972 · Vessel Strength and Wall-Thickness Deficiency · Pressure vessel · ★★★

Problem Description

SCC, leakage, fracture

Root Cause

[Mechanism] Tensile stress combined with a specific corrosive medium makes stainless steel initiate intergranular cracks at far below yield and propagate them.
[Calculation] Fluid Cl-=200ppm, weld residual stress σ=140MPa exceeds the 90MPa SCC threshold for 304 in Cl-, crack growth rate 1.2mm/month, penetrating the 8mm wall in 8000h.
[Design Omission] No residual-stress relief, no Cl- control, and no corrosion-resistant material.

Corrective Solution

1) Post-weld overall stress-relief heat treatment (620℃×2h drops σ to 60MPa), since σ>90MPa cracks and stress relief drops below the threshold — thus preventing SCC;
2) Choose 316L (Mo-bearing, Cl--resistant) over 304, since 304 is not resistant to Cl- cracking and a better steel raises resistance — thus resisting corrosion cracking;
3) Perform solution treatment (1050℃ quench), since sensitized grain boundaries crack and solution treatment homogenizes — thus reducing sensitization;
4) Hold fluid Cl-≤50ppm (blow down if exceeded), since corrosion rises with concentration and fluid control suppresses cracking — thus running to prevent cracking;
5) 100% liquid-penetrant test the weld HAZ, since cracks first show as lines and can be rejected early — thus finding cracks;
6) Run a Cl- stress-corrosion test (bent-beam 1000h), since without testing resistance is unknown and corrosion testing verifies it — thus grading resistance by data;
7) In operation, hold temperature ≤60℃ (high temperature promotes SCC), since heat accelerates cracking and temperature control suppresses it — thus running to prevent cracking;
8) Write stress relief and material selection into the process card, since the SCC root cause was missing stress relief and a non-resistant material — thus locking it in by process.

Checklist

Reference

GB/T 150.1-2011 Pressure vessels

Related model download:Understood the principle and ready to try?Go to MOULDL to download related 3D models and CAD drawings for free »