E44-264 · Valve Selection and Internal Leakage · PFA-lined butterfly valve D71F4-10 DN150 · ★★★
The lining delaminates and blisters; medium penetrates to the carbon-steel shell causing pitting and perforation, and acid seeps outside the valve
[Mechanism] The thermal-expansion mismatch between lining and substrate pushes interfacial stress above the bond strength, delaminating and blistering.
[Calculation] A void forms at the delamination and medium creeps along the gap to the shell, pitting it.
[Design Omission] Lining thickness and curing were uncontrolled and blistering wasn't inspected - the lined valve leaked.
1) Hold lining thickness ≥3mm and cure fully, since thin or under-cured lining lets interfacial stress beat the bond and delaminate, bonding it firmly;
2) Sandblast the substrate before lining to raise adhesion, since a smooth surface bonds weakly and peels, roughening for better grip;
3) Do spark testing at the works to check for blisters and pinholes, since delamination is invisible yet leaks acid, screening for breakthrough;
4) Use vacuum lining to cut interfacial voids, since bubbles are delamination crack starters, making it dense;
5) Switch strong-penetrating media to molded lining, since spun lining delaminates easily, giving a monolithic seal;
6) Periodically ultrasonic-check for blisters, since delamination is gradual, replacing early;
7) Add a shell leak-collection sump, since a perforation seeps acid outside, routing it away;
8) Put the lining process into quality control, since the un-inspected blisters were the cause, closing the loop in-process.
GB/T 37811-2019 Fluoroplastic-lined valves - General technical specifications