E44-556 · Seal Leakage · Mechanical Seal O-Ring, Fluorocarbon Rubber · ★★
Leak was 0.8L/h; the O-ring hardness was 85 Shore, over the 70 limit, with cross-section cracks and lost elasticity.
[Mechanism] The O-ring thermally ages and loses elasticity.
[Calculation] A 120℃ service > the 110℃ rating makes hardness 85 >70, loses elasticity and leaks.
[Design Omission] No temperature-rated ring, no temperature control, and no scheduled inspection — aging.
1) Replace with a temperature-rated ring (FFKM perfluoroelastomer, rated -20 to 200℃); the original fluorocarbon at 120℃ > the 110℃ rating made hardness 85 >70 Shore A, compression set >50%, lost elasticity and leaked 0.8L/h, so a temperature-rated ring does not harden and keeps elasticity to stop leak;
2) Hold chamber temperature ≤100℃ (cooling / heat sinking); every 10℃ rise roughly doubles thermal aging rate, so cool to extend life;
3) Add heat-sink fins to lower ring temperature (down 10 to 15℃); heat hardens it, so sink heat and cool the ring;
4) Choose a medium-hard ring (70 Shore A, compression set <25%); a hard ring cannot fill the face micro-gaps and leaks, so choose a soft elastic one;
5) Coat the ring with compatible grease (perfluoro grease); dry friction cracks the cross-section, so lubricate the ring to cut cracking;
6) Periodically check hardness (every 2 years, Shore meter); gradual hardening leaks, so check hardness and replace the ring;
7) Replace on a life limit (2 years / 4000h); aging leaks unpredictably, so replace by life;
8) Write the temperature-rated ring into the spec; the unselected temperature grade was the aging root cause, so gate the spec.
GB/T 3452.1-2005 Hydraulic-fluid power - Rubber O-ring seals