E44-484 · Filter Clogging and Contamination · Mine Dust-Collection Filter Bag (Polyester) · ★★
Dust-laden gas abraded the bag bottoms, holes formed, outlet dust reached 30mg>10mg, exceeding the limit
[Mechanism] High inlet gas velocity and coarse dust abraded the bags.
[Calculation] Inlet v=2m/s exceeded the 1.2 limit; abrasion rate rose 3x, bags ruptured within six months, and outlet dust reached 30mg.
[Design Omission] No pre-dedusting and high gas velocity, so the bags wore through.
1) Add a cyclone at the inlet to pre-remove coarse dust; since v=2 exceeded 1.2, abrasion tripled, and bags ruptured, pre-removal reduces wear;
2) Control inlet velocity to <1.2m/s; since high velocity causes abrasion, velocity control prevents it;
3) Add an abrasion-resistant layer at the bag bottoms; since bottoms wear first, the layer protects them;
4) Monitor outlet dust content; since a burst is detectable, dust monitoring catches it;
5) Lower filtration velocity to prevent scouring; since scouring abrades the bags, lower velocity reduces it;
6) Inspect bag bottoms periodically; since wear develops gradually, inspection tracks it;
7) Distribute gas flow evenly to prevent eccentric wear; since maldistribution causes local wear, even distribution avoids it;
8) Write pre-dedusting and velocity control into the mine-dust procedure; since dust was never pre-removed, the root cause of wear, the mine-dust procedure provides the check.
GB/T 14295-2019 Air filters