E46-005 · Welding Process & Distortion · Fillet Weld · ★★
A high current and fast travel undercut the base metal; the section was weakened and a stress concentration caused cracking
[Mechanism] Too high a current makes the arc force collapse the base-metal edge into a groove, weakening the section.
[Calculation] An undercut deeper than 0.5mm reduces the section; the stress-concentration factor rises and causes cracking.
[Design gap] The current and travel speed were not controlled.
① Control the current: adjust the welding current to specification to avoid an excessive current and a strong arc force that cause undercut
② Steady travel: reduce the travel speed so the molten pool fills the base-metal edge and no groove forms
③ Repair the undercut: repair-weld the undercut and grind it flush to restore the section size
④ Visual inspection: check the undercut depth after welding and correct it early
⑤ Magnetic-particle inspection: inspect the undercut for microcracks by MT for early detection
⑥ Welding procedure qualification: use a test plate to check whether the bead shape is acceptable
⑦ Bead-shape verification: confirm the undercut has been eliminated by visual inspection
⑧ Standardize process: write the current and travel-speed requirement into the welding procedure specification (WPS), controlling at the source
GB/T 19418-2003 Arc-welded joints in steel - Quality classification of defects