E46-084 · Heat Treatment & Stress · GCr15 Bearing Steel · ★★
GCr15 bearing steel had a hardness of HB230 after annealing (should be ≤HB207); turning wore the tool quickly and the machined surface roughness was out of tolerance.
[Mechanism] Too fast annealing cooling or too low a temperature leaves the pearlite lamellae insufficiently spheroidized, so the hardness is high and cutting is difficult.
[Calculation] A hardness of HB230 is 23 above the upper limit, increasing the cutting force and wear.
[Design gap] Neither the annealing cooling rate nor the spheroidization requirement was controlled.
① Control the annealing cooling rate: cool slowly in the furnace to ensure the pearlite spheroidizes fully
② Spheroidizing annealing: use spheroidizing annealing to obtain granular pearlite and lower the hardness
③ Hardness check: after annealing check the hardness and confirm it is ≤HB207
④ Metallographic check: examine the spheroidization grade and confirm it is acceptable
⑤ Re-anneal: re-spheroidize parts with high hardness
⑥ Tool matching: once the hardness meets the requirement select a suitable tool for machining
⑦ Quality verification: confirm machinability by hardness and metallography
⑧ Standardize process: write the annealing cooling rate into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel