E46-085 · Heat Treatment & Stress · High-Carbon Steel Die · ★★
A high-carbon steel die was ground without full tempering after quenching; a network of grinding cracks appeared on the surface, 0.3mm deep.
[Mechanism] The quenching residual stress was not relieved; grinding heat plus mechanical stress superimpose and induce surface network cracks.
[Calculation] Without tempering the residual stress exceeds 300MPa and grinding induces cracking.
[Design gap] The grinding operation was carried out without full tempering.
① Full tempering: temper fully after quenching to remove residual stress before grinding
② Control the grinding allowance: reduce the feed and depth of cut per pass to lower thermal stress
③ Adequate cooling: use plenty of coolant during grinding to avoid local overheating
④ Timely tempering: intersperse stress-relief tempering between grinding passes
⑤ Crack check: after grinding use magnetic-particle inspection to find network cracks
⑥ Rework: remove the cracking and re-temper the affected parts
⑦ Quality verification: confirm there are no grinding cracks by flaw detection
⑧ Standardize process: write temper-before-grinding into the process, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel