E46-086 · Heat Treatment & Stress · T10 Die · ★★★
A T10 die was put into storage with insufficient tempering after quenching; it cracked on its own after 10 days, with a radial fracture surface.
[Mechanism] Insufficient tempering leaves high residual stress and an unstable structure; stress release during storage causes delayed cracking.
[Calculation] Without full tempering the residual stress exceeds 400MPa and delayed cracking occurs.
[Design gap] Neither the sufficiency of tempering nor a storage check was specified.
① Full tempering: temper fully to specification after quenching to ensure a stable structure
② Double tempering: for high-carbon, high-alloy parts use two tempering cycles for a more thorough result
③ Control the tempering temperature: keep to the specified temperature and time to avoid under-tempering
④ Store and observe: after tempering let the part stand and watch for delayed cracking
⑤ Stress check: measure the residual stress by the hole-drilling method to confirm it has dropped
⑥ Flaw detection: inspect before and after storage to confirm there is no cracking
⑦ Quality verification: confirm there is no delayed cracking by stress and flaw detection
⑧ Standardize process: write tempering sufficiency into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel