E46-087 · Heat Treatment & Stress · Batch of Shafts · ★★
A batch of shafts was charged too densely; parts near the burner overheated while inner parts were underheated, the hardness within the batch varied by 8HRC, and some were not through-hardened.
[Mechanism] An overcrowded charge obstructs the furnace gas circulation, so the workpieces heat unevenly with large temperature deviations.
[Calculation] Overcrowding makes the temperature difference exceed 50℃ and scatters the properties within the batch.
[Design gap] No limits were set on the charge weight and spacing.
① Limit the charge: limit the charge weight and workpiece spacing according to the effective furnace space to keep circulation
② Arrange properly: leave gaps between workpieces and stagger them to avoid shielding
③ Furnace uniformity: periodically measure the furnace temperature uniformity and keep it within ±10℃
④ Same batch, same temperature: keep the materials and sizes of workpieces in one furnace similar and avoid mixed charging
⑤ Hardness spot check: after removal spot-check the hardness by position to confirm uniformity
⑥ Rework: reheat and re-treat underheated parts
⑦ Quality verification: confirm acceptability by the hardness scatter within the batch
⑧ Standardize process: write the charging specification into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel