E46-088 · Heat Treatment & Stress · H13 Die Steel · ★★
H13 die steel was insufficiently annealed after forging; milling produced chatter and a wavy surface, and the dimensions were 0.1mm out of tolerance.
[Mechanism] Insufficient annealing leaves an uneven structure and high residual stress; stress release during milling causes vibration.
[Calculation] High residual stress lowers the stiffness of the cutting system and causes chatter.
[Design gap] Neither adequate annealing nor stress relief was carried out.
① Full annealing: after forging carry out full spheroidizing annealing to specification for a uniform structure
② Stress relief: add a stress-relief treatment after annealing to lower the residual stress
③ Control the cooling rate: cool slowly after annealing to ensure the transformation is complete
④ Hardness check: after annealing check the hardness and structure to confirm machinability
⑤ Milling process: use suitable tooling and parameters to reduce excitation
⑥ Stress check: when necessary measure the residual stress to confirm it has dropped
⑦ Quality verification: confirm there is no chatter by the machined surface and dimensions
⑧ Standardize process: write the annealing specification into the process card, controlling at the source
GB/T 16923-2008 Normalizing and annealing of steel