E46-089 · Heat Treatment & Stress · 45 Steel Die · ★★
The borided layer on a 45 steel die was 120μm thick (should be ≤80μm); chipping and spalling occurred in service and the cavity failed.
[Mechanism] An excessively thick borided layer makes the FeB phase brittle with poor bonding to the substrate, and it spalls under load.
[Calculation] A layer thickness of 120μm is 50% over the upper limit and spalls brittlely.
[Design gap] No upper limit was set on the borided layer thickness.
① Limit the borided layer thickness: control the boriding process so the layer is ≤80μm, preferring the Fe2B phase
② Control the boriding temperature: lower it appropriately to reduce the layer thickness and brittle phase
③ Layer thickness check: after boriding measure the layer thickness; if out of tolerance, re-grind
④ Control the phase composition: adjust the process to suppress the brittle FeB phase and retain Fe2B
⑤ Rework: on spalled parts remove the layer and re-boride or repair by welding
⑥ Bond check: check the bonding between the borided layer and the substrate
⑦ Quality verification: confirm no spalling by layer thickness and bonding
⑧ Standardize process: write the borided layer thickness upper limit into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel