E46-091 · Heat Treatment & Stress · ADI Ductile Iron · ★★
The ADI ductile iron was austempered with insufficient holding; the bainite transformation was incomplete with much retained austenite, the hardness of HB300 was below the required HB350, and the strength-toughness was poor.
[Mechanism] Insufficient isothermal time leaves the austenite not fully transformed to lower bainite; the retained austenite lowers the hardness.
[Calculation] Incomplete transformation lowers the hardness by about 50HB and degrades the properties.
[Design gap] No lower limit was specified for the isothermal hold time.
① Sufficient isothermal time: ensure the austempering hold time according to wall thickness so the bainite transforms fully
② Control the isothermal temperature: keep the isothermal salt bath within the process range (e.g. 300~380℃)
③ Transformation check: measure the bainite fraction and retained austenite content by metallography to confirm completeness
④ Hardness spot check: check the hardness and confirm it is ≥HB350
⑤ Re-process: re-austemper parts with incomplete transformation
⑥ Cooling rate control: air-cool or slow-cool on removal to avoid secondary transformation
⑦ Quality verification: confirm complete transformation by metallography and hardness
⑧ Standardize process: write the isothermal time into the process card, controlling at the source
GB/T 24733-2009 Austempered ductile iron castings