E46-092 · Heat Treatment & Stress · 40Cr Part · ★★
A 40Cr part was martempered in 160℃ nitrate salt (should be 260℃); the hold near the Ms point was improper, the hardness after quenching was uneven, and some areas did not harden.
[Mechanism] A martempering temperature below Ms makes part of the martensite form unevenly during the hold, and the hardness varies after cooling.
[Calculation] The 160℃ deviation makes the cooling curve abnormal and the hardness uneven.
[Design gap] The martempering temperature was not selected according to the material.
① Choose the right martempering temperature: select it by material (e.g. Ms~Ms+50℃, about 260℃, for 40Cr)
② Control the nitrate salt temperature: keep the nitrate salt bath within the process range
③ Adequate hold: keep the martempering hold appropriate to avoid forming bainite if held too long
④ Transfer to fast cooling: after martempering transfer to a suitable medium and fast-cool to complete the martensite transformation
⑤ Hardness spot check: after quenching check the hardness distribution to confirm uniformity
⑥ Re-process: re-quench parts with uneven hardness
⑦ Quality verification: confirm uniform and acceptable hardness
⑧ Standardize process: write the martempering temperature into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel