E46-093 · Heat Treatment & Stress · 40CrNiMo Steel · ★★★
The 40CrNiMo steel was tempered at 450℃ (the blue-brittleness range); the impact energy was only 20J, below the required 80J, and it fractured brittlely in low-temperature service.
[Mechanism] Holding in the 350~550℃ temper-embrittlement range causes phosphorus and tin to segregate at the grain boundaries, and the impact toughness drops sharply.
[Calculation] Being in the embrittling temperature range lowers the impact energy by 75%.
[Design gap] The second-type temper-embrittlement temperature range was not avoided.
① Avoid the embrittling range: keep the tempering temperature out of the 350~550℃ brittle range, either above it or passed through quickly
② Fast cool through it: if the range must be crossed, pass through it quickly and fast-cool after tempering
③ Change the tempering temperature: temper above 550℃ and water-cool to eliminate embrittlement
④ Alloy control: control phosphorus, tin and other impurities to reduce segregation
⑤ Impact test: carry out an impact test to confirm the toughness meets the requirement
⑥ Metallographic check: examine the grain boundaries for anomalies
⑦ Quality verification: confirm there is no embrittlement by impact energy
⑧ Standardize process: write avoidance of the embrittling range into the process card, controlling at the source
GB/T 16924-2008 Quenching and tempering of steel