E46-095 · Heat Treatment & Stress · 6061 Aluminum Alloy · ★★
A 6061 aluminum alloy was aged only 4h after solution treatment (should be 8h); the tensile strength of 240MPa was below the required 310MPa and the component deformed under load.
[Mechanism] Insufficient aging time leaves the strengthening phases incompletely precipitated; the supersaturated solid solution is not fully precipitation-hardened.
[Calculation] Aging for 4h leaves the strength about 23% below the requirement.
[Design gap] No lower limit was specified for the aging hold time.
① Sufficient aging time: extend the artificial aging time to the process lower limit (8h for 6061) for full precipitation
② Control the aging temperature: keep the aging temperature (e.g. 160℃) stable to ensure precipitation
③ Full solution treatment: ensure the solution temperature and the quench transfer time to obtain a supersaturated solid solution
④ Hardness spot check: after aging check the hardness to confirm the strengthening effect
⑤ Tensile test: carry out a tensile test to confirm the tensile strength is ≥310MPa
⑥ Re-age: re-age insufficient parts as a remedy
⑦ Quality verification: confirm the strength meets the requirement by hardness and tensile testing
⑧ Standardize process: write the aging time into the process card, controlling at the source
GB/T 3880.1-2012 Wrought aluminium and aluminium alloy plates, sheets and strips for general engineering