E46-096 · Heat Treatment & Stress · 6061 Aluminum Alloy · ★★
A 6061 aluminum alloy was aged 12h (should be 8h) at 180℃; the strength dropped to 260MPa, below the required 310MPa, an over-aging softening.
[Mechanism] Too long and too hot an aging treatment causes the strengthening phases to agglomerate and coarsen; the dispersion drops and the alloy softens.
[Calculation] Over-aging lowers the strength by about 16%.
[Design gap] No upper limit was set on the aging treatment.
① Set an aging upper limit: keep the aging time and temperature within the process upper limit (8h/160℃ for 6061)
② Control the aging temperature: avoid overheating and keep the aging furnace temperature stable
③ Hardness spot check: after aging check the hardness to confirm it is within range
④ Metallographic check: examine the dispersion of the strengthening phases to confirm they have not coarsened
⑤ Re-solutionize and re-age: re-solutionize and re-age over-aged parts as a remedy
⑥ Furnace temperature record: record the furnace temperature curve for traceability
⑦ Quality verification: confirm the strength by hardness and tensile testing
⑧ Standardize process: write the aging upper limit into the process card, controlling at the source
GB/T 3880.1-2012 Wrought aluminium and aluminium alloy plates, sheets and strips for general engineering