E46-159 · Fastening & Anti-Loosening · Food equipment · ★★
Stainless steel bolts on food filling equipment were tightened dry; because stainless steel has a high friction coefficient and poor thermal conductivity, the engaged threads heated up and stuck during tightening, the bolt and nut seized and could not be disassembled, and had to be cut apart.
[Mechanism] The passive film on the stainless steel surface breaks down under dry friction and high temperature and cold-welds, causing adhesive wear on the threads and seizing.
[Calculation] Without lubrication the friction coefficient of stainless steel threads can exceed 0.3, and the work of tightening converts into heat that raises the local temperature above the cold-welding threshold.
[Design gap] Lubricated assembly was not specified for stainless steel fasteners.
① Thread lubrication: before assembly apply molybdenum disulfide or a food-grade anti-seize paste to the stainless steel threads to lower the friction coefficient
② Control the speed: thread in by hand or with a low-speed tool to avoid frictional heating at high speed
③ Match the alloys: use copper or a different stainless steel grade for the nut to reduce the tendency of like metals to cold-weld
④ Tighten in stages: first hand-thread fully home to confirm smoothness, then apply torque for final tightening
⑤ Avoid over-tightening: apply the design torque and never force with a cheater bar
⑥ Clean the threads: remove burrs and chips from the threads before assembly to prevent jamming
⑦ Threading verification: confirm smooth hand-threading with no jamming as proof of no seizing
⑧ Standardize process: write the requirement that stainless steel bolts must be lubricated into the assembly specification
GB/T 3098.6-2014 Mechanical properties of fasteners - Stainless steel bolts, screws and studs