E46-301 · Casting & Forging · Iron Casting · ★★
An 8mm-wall cast iron part was poured at only 1280℃ (should be above 1360℃); the thin walls did not fill completely, leaving a misrun about 30mm long, and holes were exposed after machining.
[Mechanism] At low temperature the iron is viscous and has poor fluidity; its leading edge solidifies early and blocks the flow.
[Calculation] Fluidity falls sharply as the temperature drops; at 1280℃ the fill length is about 40% less than at 1360℃.
[Design gap] No minimum pouring temperature was set by wall thickness.
① Measure the pouring temperature: measure the iron temperature with a thermocouple and return it to the furnace if below the process lower limit
② Set the temperature lower limit: determine it from wall thickness by table, using the upper end of the range for thin-wall parts
③ Control the transfer time: shorten the time from ladle to sprue to reduce heat loss
④ Condition the ladle lining: preheat and dry the ladle thoroughly to avoid excessive heat absorption
⑤ Check filling: open the flask on the first article to check for misrun, detecting problems early
⑥ Adjust the composition: raise carbon and silicon appropriately to promote graphitization and improve fluidity
⑦ Temperature verification: confirm compliance by temperature records
⑧ Standardize process: write the minimum pouring temperature into the process card, controlling at the source
GB/T 9439-2010 Grey cast iron castings