E46-302 · Casting & Forging · Cast Steel Part · ★★★
A 50kg cast steel part was poured at 1620℃ (should be 1540℃); after solidification a shrinkage cavity 40mm deep formed beneath the riser, and it was exposed after rough machining.
[Mechanism] Superheat increases liquid and solidification shrinkage; the shrinkage cavity volume grows roughly linearly with superheat.
[Calculation] Each 10℃ of superheat raises the shrinkage cavity volume by about 3%; at 1620℃ the cavity is about 24% larger than at 1540℃.
[Design gap] The tap superheat was not controlled.
① Control superheat: pour when the tap temperature is 30 to 50℃ above the liquidus, without overheating
② Measure before pouring: measure the actual temperature with a thermocouple and wait for it to cool if it exceeds the upper limit
③ Optimize the riser: size the riser by modulus to ensure the feeding path
④ Use chills: place chills at the hot spot to establish directional solidification
⑤ Check for cavities: magnetic particle inspect or ultrasonic-test after rough machining, detecting problems early
⑥ Adjust pouring: lower the pouring speed to reduce turbulence
⑦ Cavity verification: confirm the absence of shrinkage cavities by nondestructive testing
⑧ Standardize process: write the superheat into the process card, controlling at the source
GB/T 11352-2009 Cast carbon steel castings for general engineering use