E46-303 · Casting & Forging · Aluminum Alloy Housing · ★★★
An aluminum alloy housing had shrinkage porosity at a thick-wall hot spot; X-ray showed porosity covering 15% of the cross-section, and the airtightness test leaked.
[Mechanism] The hot spot solidifies last with no feeding source; the isolated liquid pockets between dendrites form shrinkage porosity.
[Calculation] Feeding is insufficient when the hot-spot modulus exceeds the riser modulus; design the riser with a modulus ratio of 1.2.
[Design gap] No modulus check was made for the hot spot.
① Modulus check: calculate the hot-spot modulus and size the riser so that M(riser) ≥ 1.2 M(hot spot)
② Add risers: place a top or side riser above the hot spot for feeding
③ Use chills: place chills around the hot spot to make it solidify first
④ Establish directional solidification: use insulating riser sleeves to extend the riser's solidification time
⑤ Airtightness test: run an airtightness or leak test on the casting, detecting problems early
⑥ X-ray check: radiograph the thick-wall areas for shrinkage porosity
⑦ Feeding verification: confirm the porosity meets specification by X-ray
⑧ Standardize process: write the riser dimensions into the process drawing, controlling at the source
GB/T 9438-2013 Aluminum-alloy castings