E46-305 · Casting & Forging · Sand Casting · ★★
The upper and lower molds were offset by 2.5mm, so the casting was misaligned at the parting line; after machining one wall was only 4mm thick (should be 8mm).
[Mechanism] During closing, the locating pins are not inserted accurately or the flask pin holes are worn, so the upper and lower molds shift relative to each other.
[Calculation] The mismatch equals the sum of the pin-hole clearance and the locating error; exceeding half the wall-thickness tolerance leaves a thin wall.
[Design gap] The closing locating accuracy was not verified.
① Check the locating pins: before closing, check the pin-to-hole fit and replace worn parts
② Add closing marks: mark a closing line or reference on the pattern, and align before closing
③ Use pin bushings: fit bushings in worn pin holes to restore accuracy
④ Spot-check the mismatch: scribe the first article to check the misalignment, detecting problems early
⑤ Control wall thickness: measure the wall-thickness distribution before machining to avoid thin walls
⑥ Die maintenance: periodically check the pattern's locating datum
⑦ Mismatch verification: confirm the misalignment is ≤0.5mm by scribing
⑧ Standardize process: write the closing locating requirements into the work instruction, controlling at the source
GB/T 6414-2017 Castings - Dimensional tolerances